Star-shaped cracks often appear on the surface of steel slabs produced by a steel plant. They are complex, shallow and deep, and clearly visible cracks similar to clusters or unclosed polygons. Such cracks are generally distributed in a band along the rolling direction, with uneven density. Shallow star-shaped cracks can be mechanically polished, but steel plates with deeper star-shaped cracks are directly judged as scrap. Tong Yunfeng from Fujian Sangang Group Co., Ltd. used a series of physical and chemical testing methods to analyze the causes of such cracks.
01 Physical and chemical testing
1.1 Macroscopic observation
If there are bubbles on the surface of the ingot, star-shaped cracks will appear on the surface of the steel plate after rolling. The steel plate sample was hot pickled with hydrochloric acid aqueous solution, and the macroscopic morphology of the star-shaped cracks of the steel plate was observed. It was found that most of the surface cracks were closed and water drop-shaped, with a slight collapse in the closed loop, and some cracks were hook-shaped, with a slight collapse inside the hook. The collapse is in the form of a water drop, an ellipse, an irregular closed loop, etc.
If there are intergranular cracks on the surface of the ingot, star-shaped cracks will also appear on the surface of the steel plate after rolling. The steel plate sample was hot pickled with hydrochloric acid aqueous solution to observe the macroscopic morphology of the star-shaped cracks on the steel plate. Most of the cracks on the surface of the sample are closed, the opening direction is inconsistent, and the polygonal characteristics are obvious.
If the low-melting-point substances (such as Cu, Sn, Pb, etc.) in the ingot are selectively oxidized or their content is high, star-shaped cracks will also appear on the surface of the steel plate after rolling. The polygonal characteristics of the cracks are most obvious, generally without hook-shaped features, and their morphology is similar to chapped cracks (see figure).
1.2 Metallographic inspection
The steel plate sample with bubbles on the surface of the ingot was observed with an optical microscope, and it was found that the tail of the star-shaped crack defect was rounded and blunt, the defect was clean, and there was no oxidation origin around it. After corrosion with a 4% volume fraction of nitric acid alcohol solution, it was found that the defect structure was ferrite + pearlite, and the grain size of the structure on both sides was obviously uneven.
The steel plate samples with intergranular cracks on the surface of the ingot were observed under an optical microscope, and a large number of secondary oxidation particles were found in the matrix around the cracks, while no secondary oxidation particles were found on the surface of the steel plate. After being corroded by a 4% volume fraction nitric acid alcohol solution, it was found that the structure at the crack was ferrite + pearlite, and decarburization was present.
Metallographic examination of the steel plate samples with selective oxidation of low-melting-point substances in the ingot or high content thereof found that the crack was about 0.07 mm deep and extended inward to 0.51 mm. A large number of secondary oxidation particles were found in the matrix around the crack and the crack extension. After being corroded by a 4% volume fraction nitric acid alcohol solution, it was found that the structure of the crack head was bainite + ferrite + a small amount of pearlite, and decarburization was present.
1.3 Energy spectrum analysis
Energy spectrum analysis of the steel plate samples with intergranular cracks on the surface of the ingot found that secondary oxidation particles were found in the matrix around the cracks, which were mainly oxidation particles containing manganese and silicon.
Energy spectrum analysis of steel plate samples with selective oxidation of low-melting-point substances in the ingot or high content thereof revealed that low-melting-point element Cu was enriched at the crack (extending and agglomerating along the direction of the crack on the sample surface). There were a large number of secondary oxidation particles in the matrix around the crack and at the extension of the crack, mainly oxidation particles containing manganese and silicon elements.
02 Comprehensive analysis
For steel plate samples with bubbles on the surface of the ingot, the morphological characteristics of its microstructure are that there is no oxidation origin around, and the grain size of the tissues on both sides is different. This indicates that the defect is a shallow surface defect, which ruptures during rolling, resulting in different grain sizes of the tissues on both sides of the defect. Generally, bubbles within 10mm of the subcutaneous area of
For steel plate samples with intergranular cracks on the surface of the ingot, there are secondary oxidation particles in the matrix around the cracks, and there is decarburization in the crack structure after corrosion. The results of energy spectrum analysis show that these oxides are mainly oxide particles containing silicon and manganese. The formation of secondary oxidation particles is very slow, and the steel plate must be placed at high temperatures and in an oxygen environment for a long time. If the steel plate is in a high-temperature environment for a short time, iron oxide can only be formed on the surface. If the finishing and rough rolling last for a short time, secondary oxidation particles cannot be generated. At the same time, because the surface of the steel plate is in an environment with a high oxygen content during the rolling process, an iron oxide protective film is quickly generated, which prevents the entry of oxygen and prevents the generation of secondary oxidation particles. This also proves that the secondary oxidation particles are not generated during the rolling process, but are generated by long-term placement in the heating furnace. Therefore, this type of star-shaped crack is an intergranular crack on the ingot.
For steel plates with selective oxidation of low-melting-point substances in the ingot or high content, the results of energy spectrum analysis show that the enrichment of low-melting-point element Cu is found at the crack, which means that the generation of the crack is related to the enrichment of Cu element.
There are two mechanisms for the enrichment of Cu on the surface and subsurface of hot-rolled steel: one is selective oxidation. The mechanism of selective oxidation is that the Cu content in the steel matrix is
03 Improvement measures
(1) Measures to reduce the star-shaped cracks in steel slabs formed by the rupture of bubbles under the billet skin are as follows:
First, the total amount of gas in the billet should be detected to determine whether the bubbles are endogenous or exogenous. For bubbles caused by high total gas volume, the total gas volume should be reduced (such as strengthening deoxidation) to prevent gas from escaping from the steel due to temperature reduction during continuous casting. For exogenous bubbles, the dryness and adaptability of the protective slag should be considered to prevent gas from entering the billet surface from the outside to form subcutaneous bubbles or pinholes.
(2) Measures to reduce star-shaped cracks in steel plates caused by intergranular cracks on the billet surface are:
Determine the process of intergranular crack generation and optimize and adjust the corresponding continuous casting process.
(3) Measures to reduce star-shaped cracks in steel plates caused by selective oxidation of low-melting-point substances on the billet surface or their high content are:
Control the content of residual elements in steel; in the high-temperature heating zone above 1100℃, ensure that the furnace is reducing or slightly reducing, or spray oxidation-reducing coatings to reduce the degree of oxidation of the steel matrix; improve the continuous casting process and improve the quality of the crystallizer to reduce the probability of damage to the crystallizer coating.
04 Conclusion
This article summarizes the causes of three types of steel plate star-shaped cracks. According to their macroscopic characteristics, microscopic characteristics, defect distribution, occurrence probability, etc., the characteristics and root causes of steel plate star cracks can be distinguished and identified to guide steel mills to quickly respond to production problems.