[Abstract] Surface slag inclusion is a common surface defect of continuous casting billets, which directly affects the surface quality of finished products. By analyzing the causes of slag inclusion on the surface of continuous casting billets, measures such as maintaining the stability of molten steel in the continuous casting mould tube, selecting appropriate protective powder and the amplitude and frequency of the ccm mould tube were formulated and implemented, so that the problem of slag inclusion on the surface of continuous casting billet was effectively controlled.
1. Introduction
In order to improve production capacity and achieve furnace-machine matching, the Tiantie Group Steelmaking Plant has carried out a series of high-efficiency transformations on the continuous casting machine, which has greatly improved the production capacity of the continuous casting machine. In order to improve the internal quality of the billets and ensure smooth production, all continuous casting machines have been implemented with full-process protective casting. However, since the implementation of protective casting, the phenomenon of slag inclusion on the surface of the billets has increased significantly, especially when pouring, stopping pouring, changing the nozzle and changing the casting speed, the phenomenon of slag inclusion on the surface of the billets is particularly prominent. In response to this phenomenon, according to the actual production situation, the steelmaking plant has formulated and implemented a series of practical and effective solutions to effectively control the slag inclusion on the surface of the continuous casting in the steelmaking plant.
2. Analysis of the causes of inclusions
2.1 Tiantie Group Steel Plant currently has three square billet continuous casting machines, one round billet continuous casting machine, and one slab continuous casting machine.
2.2 Surface slag inclusion refers to large pieces of slag embedded 2 mm to 10 mm below the surface of the billet, so it is also called subcutaneous slag inclusion. Slag inclusion is an important source of slag inclusion. If the surface slag inclusion is not removed, it will leave many defects on the surface of the finished product. For example, the black lines distributed in strips on cold-rolled thin plates are believed to be caused by calcium aluminate and Al2O3. In addition, the primary shell of the ccm mould tube is involved in slag inclusions, forming a “hot spot” on the shell. The thermal conductivity of the slag here is poor, and the solidified shell is thin, which makes it easy to cause steel leakage accidents after leaving the ccm mould tube. Slag inclusion is the most common defect in continuous casting. Only by strict control of the aspects of process and operation can the probability of slag inclusion be reduced.
2.3 When using protective casting, the fundamental reason for slag inclusion is due to the instability of the continuous casting mould tube liquid level. Therefore, inappropriate water nozzle insertion depth and sudden changes in casting speed will cause fluctuations in the mould tube liquid level, and in severe cases, lead to slag inclusions. In terms of the content of the slag inclusions, there are unmelted powdered protective slag, AlzO3 inclusions that float up and are not absorbed by the liquid slag in time, and high-viscosity protective powder that absorbs and dissolves excessive Al2O3, etc.
2.4 The influence of crystallizer liquid level fluctuation on slag inclusion is shown in Table 1.
Table 1: The influence of crystallizer liquid level fluctuation on slag inclusion
| Liquid level fluctuation range/mm | Surface slag inclusion depth/mm |
| ±20 | <2 |
| ±40 | <4 |
| >40 | <7 |
Keeping the liquid level fluctuation less than ±10mm can effectively control the surface slag inclusion. Therefore, it is very important to select a sensitive and reliable automatic control system for the copper mould tube liquid level to control the liquid level fluctuation within the allowable range (such as ±3 mm~±5 mm) to prevent surface slag inclusion.
The immersion depth of the submerged nozzle has a great influence on the slag inclusion on the surface of the billet. If the immersion depth of the nozzle is too shallow (<100mm), the billet will have a serious slag roll; if the immersion depth is too deep, the protective powder will not melt evenly. Selecting an immersion depth of 100 mm~150 mm can reduce surface slag inclusion. For specific impact conditions, please refer to Table 2.
In addition, poor refractory quality, poor performance of protective powder, unreasonable vibration parameters, improper pouring operation, etc. can also cause slag inclusion in the billet.
Table 2: Influence of nozzle immersion depth on slag roll
| Immersion depth/mm | Slag spot index |
| ≤80 | 2.85 |
| 85~100 | 1.65 |
| 105~120 | 1.15 |
| 125~140 | 0.95 |
| >145 | 0.85 |
3. Solutions
To prevent slag from rolling inside the copper mould tube, the following measures are taken to reduce the slag inclusion phenomenon on the surface of the continuous casting billet in the steel plant.
3.1 Ensure the stability of the liquid level
The liquid level fluctuation is as small as possible (<±5mm). For this reason, the steel plant adopts a caesium source (Cs137) mould tube liquid level automatic control system to control the mould tube liquid level fluctuation within ±2 mm, ensuring the stability of the mould tube liquid level. At the same time, an automatic protective powder-adding system is adopted to add protective powder at a fixed time and quantity and to ensure the uniformity of protective powder addition.
Automatic continuous casting powder adding system >>
3.2 Ensure the appropriate immersion depth of the submerged nozzle
The immersion depth is preferably 100 mm~150 mm. Most of the tundishes in the steel plant have been used for too long, and the tundish body has undergone a certain degree of deformation. At the same time, after the modification of the tundish car, the height increased, resulting in the original 580 mm long immersion nozzle not being able to meet the immersion depth requirement of 100 mm ~ 150 mm, and the actual immersion depth was only 50 mm ~ 80 mm. The phenomenon of the liquid surface of the copper mould tube often tumbles during use, increasing the probability of slag inclusion on the surface of the billet. After actually measuring the distance from the bottom of the tundish to the copper mould tube, the length of the immersion nozzle was increased to 640 mm, ensuring that the immersion depth of the nozzle was within a reasonable range and the liquid surface of the copper mould tube no longer tumbled.
3.3 Selecting a suitable protective powder
The viscosity of the protective powder is one of the important properties that determines the consumption and uniform penetration. In order to improve uniform heat transfer and good lubrication under high pulling speed conditions, maintain sufficient liquid powder layer thickness and protective powder consumption, measures should be taken to reduce the viscosity. However, too low a protective powder viscosity will reduce the protective powder’s ability to resist molten steel mixing and increase the probability of slag entanglement. Therefore, the viscosity of the protective powder should be appropriately increased while ensuring that the protective powder can flow smoothly into the copper mould tube and the billet to form a continuous slag film. Ensuring that the thickness of the liquid slag layer is between 8 mm and 12 mm can prevent unmelted slag from being drawn into the billet shell.
3.4 Basicity of protective powder
The basicity of protective powder is an important indicator, and it should be adjusted according to the solidification characteristics of each steel grade. For low-carbon aluminium-killed steel, it is best to use protective powder with a slightly higher basicity and the lowest original Al2O3 content, and appropriately increase the consumption of protective powder to make the liquid slag layer update faster and enhance the absorption and dissolution of Al2O3.
Through exchanges and discussions with protective powder manufacturers, the physical and chemical indicators of protective powder for various steel grades were adjusted to make the powder have more suitable viscosity, melting speed and liquid slag layer thickness, ensure that the protective powder can flow evenly and stably along the four walls of the copper mould tube, and have a better ability to absorb floating inclusions. The physical and chemical indicators of protective powder before and after adjustment of a certain steel grade are shown in Tables 3 and 4.
Table 3: Before adjusting
| SiO2/% | CaO/% | Al2O3/% | MgO/% | Melting point/℃ | Melting rate/1300℃ S | Viscosity/1300℃ Pa▪S |
| 33.0±3.5 | 31.5±3.5 | ≤7.5 | ≤8.0 | 1130±30 | ≤55 | 0.15±0.05 |
Table 4: After adjusting
| SiO2/% | CaO/% | Al2O3/% | MgO/% | Melting point/℃ | Melting rate/1300℃ S | Viscosity/1300℃ Pa▪S |
| 29.5±3.5 | 36.5±3.5 | ≤6.0 | ≤6.0 | 1080±30 | ≤39 | 0.30±0.05 |
By adjusting the physical and chemical indicators of the protective powder, the ability of the protective powder to resist the mixing of molten steel is enhanced while ensuring its lubrication performance.
3.5 Selecting the appropriate amplitude and frequency
During the steel casting process, the liquid protective slag flows into the gap between the copper mould tube and the shell through the channel formed between the slag ring and the very thin meniscus shell. During the positive slip time of the copper mould tube (the downward speed of the tube is less than the pulling speed), the channel is unobstructed and the protective powder will flow in normally.
However, during the negative slip time (the downward speed of the copper mould tube is greater than the pulling speed), the inflow of protective powder will be abnormal because the slag ring collides with the meniscus shell of the tube and bends it. During this period of time, the vibration marks of the casting are also formed. Therefore, under the condition of ensuring a certain negative slip time (to ensure smooth demoulding), increasing the positive slip time and ensuring a reasonable amount of protective powder can reduce the surface slag inclusion phenomenon and reduce the depth of vibration marks.
Steel mills set different amplitudes according to the needs of copper mould tubes with different sections. For example, the tube with a cross-section of 120 mm x 120 mm uses an amplitude of ± 5 mm, and the copper mould tube with a cross-section of 150 mm x 150 mm uses an amplitude of ± 4 mm.
The vibration frequency adopts the control model of f = av + b, and different vibration constants are used according to different cross sections, and the minimum vibration frequency is set when the pulling speed drops to a certain value (such as the minimum vibration frequency of the 160×220 cross section is 80 times/min) to ensure the demoulding and lubrication of the casting billet at low pulling speed under abnormal conditions.
Reasonable vibration parameters ensure a reasonable amount of protective powder and reduce the surface slag inclusion phenomenon.
3.6 Improve the quality of refractory materials
The erosion products caused by poor quality of refractory materials are also one of the reasons for surface slag inclusion. Therefore, it is stipulated that when producing steel with high manganese content, aluminium carbon middle package immersion nozzles should be used to extend the service life of the nozzles. Replace damaged immersion nozzles in time to reduce slag rolls. Promote the use of smear material tundish and dry material tundish, and use a slag retaining wall and slag retaining dam to reduce the impact of tundish refractory and molten steel inclusions on the surface of the billet.
3.7 Ensure appropriate pouring temperature and pulling speed
Temperature that is too low is prone to slag rolling, and a temperature that is too high will cause other defects or accidents. Too high or too low pulling speed will increase the probability of slag rolling.
By strengthening converter endpoint control, red envelope steelmaking, and strengthening production organization and coordination, reasonable molten steel superheat and molten steel connection are guaranteed, and the pouring temperature and pulling speed tend to be stable.
3.8 Use electromagnetic force to control the flow of molten steel
In order to improve the internal and external quality of the ingot, the steelmaking plant has added a copper mould tube electromagnetic stirring system. The electromagnetic stirring system can reduce the impact depth of the molten steel and make the molten steel produce forced convection circulation. In addition to improving the internal defects such as central looseness and shrinkage of the billet, it can also eliminate subcutaneous pores and surface slag inclusions and improve surface quality.
3.9 Standardize the operation process and use the correct operation method
3.9.1 When the liquid level of the crystallizer fluctuates abnormally, the protective powder should be added after the liquid level stabilizes.
3.9.2 The protective powder shall not be directly pushed to the corner of the copper mould tube, and the protective powder shall be evenly sprinkled on the liquid surface.
3.9.3 The slag blocks or slag rings appearing on the surface of the molten steel shall be removed in time. When removing the slag blocks or slag rings, the direction shall be pointed to avoid the molten steel rolling slag.
3.9.4 When the tundish is opened for pouring or the nozzle is replaced, the protective powder must be added after the molten steel surface is immersed in the nozzle.
3.9.5 The protective powder should be added frequently and thinly to ensure that a layer of new slag is always covered on the slag layer.
3.9.6 The liquid surface of the copper mould tube should ensure that the molten steel is not exposed during normal pouring. The slag surface is bright red on the four walls of the tube, and the other places are the original colour of the protective powder. The thickness of the slag layer (liquid slag plus powder slag) should be controlled to 35mm~40mm.
3.9.7 When using an automatic powder feeder, pay attention to fine-tuning the addition position after starting to ensure that it meets the slag addition requirements.
4. Implementation effect
When using protective casting, the fundamental reason for slag inclusion is due to the instability of the copper mould tube liquid surface. According to the actual production situation of the steel mill, by taking the above measures, the slag inclusion phenomenon on the surface of the steel mill’s billet is effectively controlled, and the quality of the steel mill’s billet, especially the slab, has been greatly improved. The qualified rate has increased from 97.18% in 2006 to 98.30% in 2007. The improvement of billet quality has reduced the number of scrap and finishing products, reduced production costs, and created greater economic and social benefits for the company.